Through first-principles calculations coupled with phonon Boltzmann transport and scattering-aware electron transport, this study obtains pronounced lattice transport anisotropy and quantified thermoelectric response results for tetragonal GeS₂ and GeSe₂.
The thermal transport calculations for layered tetragonal GeS₂ and GeSe₂ cover the 300–800 K temperature range, with carrier concentrations set from 10¹⁸ to 10²² cm⁻³. Post-processing for the two materials was performed using AMSET dense interpolation grids of 81×81×25 and 81×81×27, respectively; these grids were generated from converted dense non-self-consistent band structures and are independent of the self-consistent/non-self-consistent k-point grids of Quantum ESPRESSO.
The converted transport bands under the PBE functional give a band gap of 0.99 eV for GeS₂, while GeSe₂ is nearly gap-closed on the dense transport grid, exhibiting only about 0.015 eV of band overlap. This near-zero-gap PBE result limits the precision of quantitative interpretation of GeSe₂'s high-temperature results.
The quantitative thermodynamic figure-of-merit calculations in this work combine the electron transport coefficients output by AMSET with the lattice thermal conductivity tensor obtained within the ShengBTE relaxation-time approximation framework, while the band structure obtained from HSE03 hybrid functional combined with Wannier interpolation serves as an independent constant-relaxation-time reference benchmark. All key numerical settings are summarized in supplementary material tables and can support reproduction of the published results.
This study first completed mechanical stability verification of layered tetragonal GeS₂ and GeSe₂; all calculated elastic constants satisfy the Born mechanical stability criteria for tetragonal crystals, confirming that the optimized crystal structures of both materials are mechanically stable under small homogeneous strains. The study also observed strong anisotropy in the stiffness of both compounds: in-plane elastic constants are far larger than the cross-plane ones, a feature fully consistent with the weaker resistance to deformation along the stacking direction of the layered tetragonal framework.
Based on phonon Boltzmann transport calculations, the study explicitly observes significant lattice transport anisotropy in this system, obtaining complete quantitative results of in-plane and cross-plane lattice thermal conductivities of both materials at two typical temperatures of 300 K and 800 K within the relaxation-time approximation framework.
The electronic band calculations of this study adopt a comparative scheme of PBE functional versus HSE03 hybrid functional, obtaining band dispersions along high-symmetry paths after Wannier interpolation. The PBE calculations yield band gaps of 0.98 eV for GeS₂ and 0.08 eV for GeSe₂; after processing through the HSE03/Wannier route, the gaps are raised to 2.48 eV and 1.23 eV, respectively. The dense PBE grid used for AMSET calculations pushes GeSe₂'s gap further toward zero. The consistent results of the two PBE descriptions indicate that under semi-local functionals GeSe₂ lies near the semiconductor–semimetal boundary, and the correction from the HSE03 functional mainly consists of a rigid upward shift of the conduction band.
All lattice thermal conductivities used in this study's thermoelectric analysis were solved via ShengBTE within the relaxation-time approximation (RTA), covering three typical temperatures of 300 K, 500 K, and 800 K, with independent conductivity components output for the in-plane direction and the cross-plane direction . Their ratio serves as a quantitative indicator of the degree of anisotropy and is directly incorporated into the subsequent electron–phonon coupled transport calculation workflow.
The Hill-averaged elastic parameters of the two layered tetragonal compounds show that GeS₂ has a bulk modulus B of 33.61 GPa, shear modulus G of 19.72 GPa, and Young's modulus E of 49.17 GPa, while the corresponding values for GeSe₂ are 37.43 GPa, 18.37 GPa, and 46.60 GPa. These moderate values indicate that both materials are mechanically softer than three-dimensional densely covalently bonded solids; their Pugh ratios are 1.70 and 2.04, respectively, with GeS₂ slightly below the empirical ductile–brittle threshold of 1.75 and GeSe₂ above it, exhibiting an overall more ductile average mechanical response.
The core result of the study is an extremely strong anisotropic separation between in-plane and cross-plane heat flow. At 300 K, the GeS₂ lattice thermal conductivity computed with the Sheng-BTE RTA method has an in-plane component of 26.86 W m⁻¹ K⁻¹, while the cross-plane c-direction component is only 1.19 W m⁻¹ K⁻¹; the corresponding values for GeSe₂ are 18.74 W m⁻¹ K⁻¹ and 1.52 W m⁻¹ K⁻¹, respectively.
When the temperature rises to 800 K, the cross-plane lattice thermal conductivities of both materials decrease further to 0.46 W m⁻¹ K⁻¹ and 0.58 W m⁻¹ K⁻¹, respectively. This significantly suppressed cross-plane thermal transport effect arises from the combined action of the materials' layered tetrahedral framework structure, shear softening, low-frequency heat-carrying phonons, and moderate anharmonicity.
By coupling the ShengBTE RTA lattice tensors with the AMSET electron transport coefficients, this study completed quantitative calculations of the full-direction thermoelectric performance of both germanium chalcogenides. All zT results at 800 K are taken directly from sampling points on the carrier concentration grid, not interpolated theoretical optima: GeS₂'s n-type cross-plane transport achieves the highest zT value in that branch, 0.257, at a carrier concentration of 10¹⁹ cm⁻³, and GeSe₂'s p-type cross-plane transport achieves the highest zT value in that branch, 0.066, at a carrier concentration of 3×10²⁰ cm⁻³.